Tile data sheets are full of standard numbers: ISO 13006, EN 14411, ISO 10545-3, R10, PTV 36, DCOF 0.42. This page explains what each one means, which ones your market and your project actually need, and what to ask for before you order. One rule applies throughout: a value only counts if it comes from a test report for that product and finish. We publish values on our product pages only from reports we hold; everything else says “test report on request”.
Key takeaways
- ISO 13006 (internationally) and EN 14411 (in Europe) classify tiles and set the minimum requirements; ISO 10545 is the set of test methods used to check them.
- Porcelain and vitrified tiles are dry-pressed tiles with water absorption of 0.5% or less — group BIa.
- For CE marking in the EU, the producing manufacturer issues a Declaration of Performance against the harmonised EN 14411.
- Slip resistance has no pass mark in ISO 13006: ask for the method your market uses — R9–R13 ramp, pendulum (PTV), DCOF or AS 4586 classes.
- Ask for the test report for the exact product, finish and thickness, with the laboratory, date and report number.
ISO 13006: how tiles are classified
ISO 13006:2018 defines ceramic tiles, classifies them and sets their characteristics and marking. It sorts tiles by two things: how they are formed — A for extruded, B for dry-pressed — and how much water the fired body absorbs (E).
| Group | Water absorption (E) | Common trade names |
|---|---|---|
| BIa | E ≤ 0.5% | Porcelain, vitrified, GVT / PGVT, full body, double charge, porcelain slabs |
| BIb | 0.5% < E ≤ 3% | Semi-vitrified / stoneware |
| BIIa | 3% < E ≤ 6% | Stoneware |
| BIIb | 6% < E ≤ 10% | Semi-stoneware |
| BIII | E > 10% | Ceramic wall tiles |
For group BIa, the main requirements include an average water absorption of no more than 0.5% (no single tile above 0.6%), a breaking strength of at least 1,300 N for tiles 7.5 mm thick or more, and a modulus of rupture of at least 35 N/mm² on average. Length and width may vary by about ±0.6% of the work size and thickness by ±5%, and at least 95% of tiles must be free of visible surface defects. Each product page has a table of these requirements with the matching ISO 10545 method; the “product result” column fills in only from a report we hold.
EN 14411 and CE marking in Europe
EN 14411 is the European counterpart of ISO 13006, with the same groups. It matters most because it is the harmonised standard behind CE marking: tiles placed on the EU market need CE marking and a Declaration of Performance (DoP) drawn up by the producing manufacturer. The edition cited for CE marking is EN 14411:2012 — the later 2016 text has not been cited, so check that a DoP refers to the right edition. The EU’s new Construction Products Regulation (EU) 2024/3110 applies from 8 January 2026, but tiles keep the existing DoP route until a new harmonised specification is adopted. The UK uses the same standard for UKCA marking. See our EU market guide for duties and importer obligations.
ISO 10545: the test methods
ISO 10545 is a series of test methods, each published as a separate part. A test report should name the part used for every value.
| Part | What it tests | When it matters |
|---|---|---|
| ISO 10545-2 | Dimensions and surface quality (size, thickness, straightness, flatness, defects) | Every order; large formats and thin joints |
| ISO 10545-3 | Water absorption | Confirms the group (BIa for porcelain); frost and outdoor use |
| ISO 10545-4 | Modulus of rupture and breaking strength | Floors, commercial traffic, thin tiles |
| ISO 10545-6 | Deep abrasion of unglazed tiles | Full body and unglazed floors |
| ISO 10545-7 | Surface abrasion of glazed tiles (PEI class 0–5) | Glazed floors: the higher the class, the heavier the foot traffic |
| ISO 10545-8 | Linear thermal expansion | Underfloor heating, facades, sun-exposed areas |
| ISO 10545-9 | Thermal shock resistance | Kitchens, outdoor areas |
| ISO 10545-10 | Moisture expansion | Mainly higher-absorption tiles |
| ISO 10545-11 | Crazing resistance of glazed tiles | Glazed wall and floor tiles |
| ISO 10545-12 | Frost resistance | Any outdoor use where it freezes |
| ISO 10545-13 | Chemical resistance | Kitchens, labs, pools, cleaning agents |
| ISO 10545-14 | Stain resistance | Polished and glazed surfaces in homes, hotels and restaurants |
| ISO 10545-16 | Small colour differences | Plain colours; see shade variation |
Slip resistance: four systems, no conversion
ISO 13006 and EN 14411 set no slip pass mark — the value and the method are declared. Markets use different tests, and there is no exact conversion between them, so ask for the one your project’s rules use.
| System | How it is tested | Classes or threshold | Used in |
|---|---|---|---|
| R9–R13 (ramp, shod) | A person in safety boots walks on an oiled ramp; the angle where walking becomes unsafe sets the class. Originally DIN 51130, now part of EN 16165:2021. | R9 6–10°, R10 >10–19°, R11 >19–27°, R12 >27–35°, R13 >35° | Germany, much of Europe, the GCC, India |
| A / B / C (ramp, barefoot) | Bare feet on a ramp wet with soapy water (originally DIN 51097, now in EN 16165). | A ≥12°, B ≥18°, C ≥24° (C is the most slip-resistant) | Showers, changing rooms, pool surrounds |
| Pendulum test value (PTV) | A pendulum swings a rubber slider over the wet surface (BS EN 16165, which replaced BS 7976). Slider 96 for shoes, Slider 55 for bare feet. | UK guidance: 36+ low slip potential, 25–35 moderate, 0–24 high | United Kingdom, Ireland |
| DCOF | A tribometer drags a rubber test foot over the wet tile (ANSI A326.3). | ≥ 0.42 for level interior floors expected to be walked on when wet — not automatically suitable for every project | United States |
| AS 4586 | Wet pendulum classes P0–P5; ramp classes for some situations. | P0 (lowest) to P5 (highest) | Australia |
Higher slip resistance usually means a rougher surface that is harder to clean, so choose the lowest class that is safe for the area — and remember that a polished and a matt tile of the same design are different products with different results. Our guide to slip ratings R9–R13 suggests classes by area.
What to ask for before you order
- A test report per product, finish and thickness — with the laboratory, the date, the report number and the ISO 10545 part for each value.
- For the EU: the manufacturer’s Declaration of Performance against EN 14411. For the UK: the UKCA declaration.
- The slip test your market uses (R-class, PTV with slider, DCOF or AS 4586 class), for the exact finish.
- The PEI class for glazed floor tiles, and frost resistance for anything outdoors.
- Any market conformity scheme your country requires — for example the Saudi Quality Mark and SABER, Thailand’s TIS 2508 licence or a PVoC certificate in East Africa. Our market guides list them.
- Who holds each certificate: plant certificates belong to the producing factory, which is named on our documents.
Reports are shared per product on request with your quotation, and an independent inspection before loading is always welcome — see our pre-shipment inspection guide. For colour lots and size sorting, read shade variation and calibre.